What Is Undercut in Welding? Causes, Limits and How to Fix It

What is undercut in welding? A groove melted beside the weld toe. Learn the causes in MIG and stick welding, how codes limit its depth, and how to repair it.
Source: AISC Shapes Database v16.0Imperial & metric
What Is Undercut in Welding? Causes, Limits and How to Fix It

Undercut is a groove melted into the base metal along the edge (toe) of a weld that the filler metal did not fill back in. It is usually caused by too much voltage or current, travelling too fast, or holding the gun or rod at the wrong angle, and it is fixed by slowing down, turning the heat down and aiming the arc so the metal fills both sides of the joint.

This guide shows what undercut looks like, why it matters on structural steel, the most common causes for MIG and stick welding, how welding codes limit it, and how to repair it. Sources were checked on November 10, 2026.

What Undercut Looks Like

TWI, the UK welding research institute, defines undercut in its review of weld shape imperfections as “an irregular groove at the toe of a run in the parent metal”, and calls it probably the most common shape imperfection in arc and gas welding. Look along the line where the weld bead meets the plate. If you see a notch or shadowed channel running beside the bead, and you can catch a fingernail in it, that is undercut.

Cross-section of a fillet weld in a T-joint. A vertical plate stands on a horizontal plate and a triangular fillet weld fills the corner. At the top toe of the weld, on the vertical plate, a small groove has been melted into the plate and left unfilled. This groove is the undercut. The section of plate behind it is thinner than the rest of the plate. undercut groove at the toe fillet weld vertical plate horizontal plate
Undercut on a horizontal fillet weld. The arc melted a groove into the upper plate that the filler did not fill, leaving a thinner section and a sharp notch.

It is easy to confuse with two other defects:

  • Underfill: the weld itself is low, below the surface of the plate. The base metal is not grooved, the joint just was not filled.
  • Overlap (cold lap): the opposite problem. Weld metal rolls over onto the plate without fusing to it.

Why Undercut Matters

Undercut takes material away from the base metal right where the stress is highest. It does two things:

  • Reduces the section. The plate is thinner along the groove, so it carries less load there.
  • Creates a notch. A sharp groove concentrates stress. Under repeated loads (vibration, cranes, traffic, wind), fatigue cracks can start at a notch long before the member is anywhere near its static capacity.

In a multi-pass weld there is a third problem. TWI notes that undercut can form at the toe of each pass, and slag can get trapped in it when the next pass goes over the top, which leaves a hidden inclusion inside the weld.

On a garden gate, a shallow undercut is cosmetic. On a beam-to-column moment connection, a crane runway or a stair stringer, it is a defect the inspector will measure.

What Causes Undercut

The basic cause is the same in every process: the arc melts more base metal than the filler can replace. TWI sums up the usual cause as a wide spreading arc (high arc voltage) with too little fill (low current or high travel speed). The specific causes:

CauseWhat happensFix
Voltage or arc length too highA wide arc melts the plate edges beyond the beadLower the voltage (MIG) or hold a shorter arc (stick, TIG)
Current too highToo much heat at the toes, and you have to travel fast to keep upTurn the amperage or wire speed down to suit the joint
Travel speed too fastThe groove is melted but not enough filler is laid in to fill itSlow down; on MIG, also raise the wire feed speed to add metal
Wrong gun or electrode angleThe arc is aimed at one plate and gouges itPoint the arc so the heat is shared by both members
Weave without a pause at the edgesThe sides of the bead are melted and left thinPause briefly at each side of the weave so the metal fills the toe
Arc blowMagnetic forces push the arc to one side, often near the end of a jointMove the work clamp to a different spot
Welding positionGravity pulls the pool down, leaving the top toe of a horizontal fillet starvedUse a smaller bead and angle the gun up slightly toward the top plate
Causes from the TWI shape imperfection review and Hobart Brothers’ MIG troubleshooting guide.

Undercut in MIG welding

Hobart Brothers’ MIG troubleshooting guide for solid and metal-cored wire lists excessive voltage, travel speed that is too fast without enough filler metal, and an incorrect gun angle that focuses the arc on the bottom plate. Its fix is to reduce travel speed and increase wire feed speed so there is enough filler to fill the joint, and to pause at the sides when weaving. When undercut shows up only toward the end of a joint, it points to arc blow and suggests moving the work clamp.

Undercut in stick welding

In stick welding the arc length is in your hand, so a long arc is the usual culprit, along with running the rod too hot for the plate. With a low-hydrogen rod such as 7018, hold a tight arc and keep the rod angle steady. Vertical-up welds are prone to undercut at the edges of the weave if you do not pause at each side.

How Much Undercut Is Allowed?

Most welding codes accept some undercut, as long as it is shallow and the transition is smooth. The exact limit depends on the code, the thickness of the material, whether the structure sees repeated (cyclic) loading, and the direction of stress relative to the undercut.

TWI’s review gives a feel for the numbers: the international standard BS EN ISO 5817 allows from 0.5 mm (its most stringent level) to 1 mm (its moderate level) for material thicker than 3 mm, and AWS D1.1 allows 1 mm (about 1/32 in). In the US, structural steel welding is governed by AWS D1.1, Structural Welding Code – Steel. Its visual inspection acceptance table sets tighter limits for cyclically loaded members and allows a little more over short lengths on static work, so check the table in the edition your project specifies rather than relying on a single number.

TWI also points out that measuring undercut is not easy, because mill scale, spatter and surface irregularities get in the way. Inspectors use a weld gauge with a depth pointer, after the area has been cleaned.

How to Repair Undercut

There are two standard repairs, and TWI names both:

  1. Blend grinding: for shallow undercut, grind the groove out to a smooth, gradual profile so the notch is gone. This removes a little more base metal, so it only works when the remaining thickness is still acceptable.
  2. An additional weld bead: for deeper undercut, clean the groove and lay a small bead along the toe to fill it, then check that the new toe blends smoothly into the plate.

On code work, repairs follow the project’s welding procedures and are re-inspected. On a fabricated beam or column, the fabricator’s quality program decides who does the repair and who signs it off; see structural steel fabrication for how that process runs. Do not cover undercut with paint or filler and call it done.

Quick Checklist to Prevent Undercut

  • Set voltage and wire speed (or amperage) for the plate thickness, starting from the wire or rod maker’s chart.
  • Keep the arc short and steady.
  • Travel only as fast as the joint fills; watch the toes, not the arc.
  • Aim the arc so both members melt evenly; on horizontal fillets, favor the top plate slightly.
  • When weaving, pause at each edge.
  • Clean mill scale, rust and oil off the joint so you can see the toe while you weld.

Weld size and type for a structural joint are shown on the drawings with weld symbols. Whether a weld with a defect is still adequate for its load is a question for a licensed structural engineer and the inspector, not a judgment to make by eye.

Undercut FAQ

What is the main cause of undercut in welding?

Too much arc energy at the edge of the weld with too little filler to replace what was melted. In practice that means voltage or current too high, a long arc, travelling too fast or a poor gun or rod angle.

Is undercut a serious weld defect?

It depends on its depth and on the load. Shallow undercut within code limits is accepted on most structural work. Deeper undercut, or undercut on members that see repeated loading, can start fatigue cracks and must be repaired.

What is the difference between undercut and underfill?

Undercut is a groove cut into the base metal beside the weld. Underfill is a weld face that sits below the plate surface because the joint was not filled. Both reduce the section, but they have different causes.

Can you grind out undercut?

Yes, if it is shallow. Blend grinding to a smooth profile is one of the two standard repairs. If grinding would leave the plate too thin, fill the groove with an extra weld bead instead.

How do you stop undercut on a vertical weld?

Turn the heat down slightly, keep a short arc, and pause at each side of the weave so the metal fills the edges before you move across. Moving too fast through the sides is the usual cause.

Reference information only, not engineering advice. Disclaimer.

Look up any steel beam size

Search all 339 AISC W, S and HP shapes, compare sizes by depth and work out total weight in seconds.