4140 Steel: Composition, Strength, Heat Treatment and Uses

4140 steel is a chromoly alloy steel for shafts, gears and bolts. Composition, strength, heat treatment temperatures, welding precautions and equivalent grades.
Source: AISC Shapes Database v16.0Imperial & metric
4140 Steel: Composition, Strength, Heat Treatment and Uses

4140 steel is a chromium-molybdenum low alloy steel with about 0.40% carbon, made to be hardened and tempered for high strength and toughness. It is the standard choice for shafts, spindles, gears, studs and high-strength bolts, where plain carbon steel is not strong enough, but it is not a structural shape steel and is not used for building beams.

Below you will find 4140’s chemical composition, typical mechanical properties in the supplied condition, heat treatment temperatures, welding precautions, equivalent grades and how it compares with the structural steels used for beams. Figures come from published mill and distributor data sheets checked on November 19, 2026.

What the Name 4140 Means

4140 uses the four-digit AISI/SAE numbering system for carbon and alloy steels. The first two digits identify the alloy family, and the last two give the nominal carbon content in hundredths of a percent:

  • 41xx: the chromium-molybdenum family, often shortened to “chromoly” or “Cr-Mo.”
  • xx40: about 0.40% carbon.

So 4130 is the same family with about 0.30% carbon, and 4140 has more carbon, which lets it reach higher hardness after heat treatment at the cost of being harder to weld. If you are new to how carbon content changes steel, our guide to mild steel explains the low-carbon end of the scale.

4140 Chemical Composition

Exact limits vary slightly between the standards a bar is certified to, so two published data sheets are shown side by side. The Atlas Steels 4140 grade data sheet gives ranges for material certified to AS1444, ASTM A434 (A29) and EN 10083 42CrMo4. The voestalpine High Performance Metals 4140 data sheet gives maximum values.

ElementAtlas Steels range (%)voestalpine max (%)What it does
Carbon (C)0.37 to 0.440.40Sets the hardness reachable by quenching
Manganese (Mn)0.65 to 1.101.00Adds hardenability and strength
Silicon (Si)0.10 to 0.350.40Deoxidizer, adds some strength
Chromium (Cr)0.75 to 1.201.10Deeper hardening, wear resistance
Molybdenum (Mo)0.15 to 0.300.30Hardenability; reduces temper brittleness
Phosphorus (P)0.040 max0.035Impurity, kept low
Sulfur (S)0.040 max0.035Impurity, kept low
Sources: Atlas Steels grade data sheet (revised Sept 2021) and voestalpine HPM Australia data sheet (2026). Always check the mill certificate for the actual heat.

With roughly 1% chromium and under 0.3% molybdenum, 4140 is a low alloy steel, not a stainless steel. It will rust if left unprotected, so the same rules covered in our carbon steel vs stainless steel comparison apply.

4140 Mechanical Properties

4140 bar is usually sold already hardened and tempered (often called “4140 HT” or “pre-hard”) to a level that is strong but still machinable. Strength drops a little in bigger diameters because the center of a thick bar cools more slowly during quenching.

Bar diameterTensile strength0.2% proof (yield) strength, minElongation, minHardness
Up to 180 mm (about 7 in), Condition U930 to 1,080 MPa (135 to 157 ksi)740 MPa (107 ksi)12%269 to 331 HB
Over 180 to 250 mm (about 7 to 10 in), Condition T850 to 1,000 MPa (123 to 145 ksi)665 MPa (96 ksi)13%248 to 302 HB
Over 250 to 450 mm, Condition T850 to 1,000 MPa (123 to 145 ksi)665 MPa (96 ksi)13%248 to 302 HB
Hardened and tempered supply condition per AS1444, from the Atlas Steels 4140 data sheet. The voestalpine sheet lists the same values for 10 to 100 mm and 101 to 250 mm bars. ksi values converted at 1 ksi = 6.895 MPa and rounded.

Annealed 4140, sold for parts that will be heat treated after machining, is much softer and weaker than these figures. Ask the supplier which condition you are buying. For what yield and tensile strength actually mean, see our explainer on the yield strength of steel.

Heat Treating 4140

Heat treatment is the whole point of 4140. In the annealed state it offers little over a plain carbon steel; hardened and tempered, it is far stronger. The ranges below are from the Atlas Steels data sheet, with Fahrenheit conversions rounded.

Vertical temperature scale from 0 to 1000 degrees Celsius showing 4140 heat treatment bands. Hardening at 850 to 860 degrees C with an oil quench is at the top. Below it, the normal tempering band runs from 500 to 680 degrees C. Nitriding at about 510 degrees C sits inside that band. Lower down, a red band from 230 to 370 degrees C is marked avoid, temper brittleness. 0 °C 500 °C 1000 °C Harden 850-860 °C, oil quench Temper 500-680 °C (normal range) Nitride about 510 °C Avoid 230-370 °C (temper brittleness)
4140 heat treatment bands on a 0 to 1000 °C scale, from the Atlas Steels grade data sheet. Not a procedure; use a qualified heat treater.
  • Hardening: heat slowly to 850 to 860 °C (about 1,560 to 1,580 °F), hold until uniform, then quench in oil or a polymer quenchant with a similar cooling rate.
  • Tempering: re-heat while still warm and hold one hour per 25 mm (1 in) of section, two hours minimum. For yield strengths below 1,380 MPa (about 200 ksi), temper between 500 and 680 °C (about 930 to 1,255 °F).
  • Avoid 230 to 370 °C (about 445 to 700 °F): holding in this range can cause temper embrittlement, sometimes called blue brittleness.
  • Nitriding: about 510 °C (950 °F) for 10 to 60 hours depending on case depth, giving a surface hardness of 600 to 650 HV.
  • Induction or flame hardening: the surface can be hardened to about 58 HRC (typical).

The voestalpine sheet notes that the molybdenum addition keeps 4140 from being susceptible to temper brittleness in normal practice.

Can You Weld 4140?

Only with care, and generally it is avoided. The Atlas data sheet says welding is not recommended because of the likelihood of quench cracking. The carbon and alloy content that let 4140 harden in an oil quench also let the weld zone harden as it cools in air, which makes it brittle and prone to hydrogen cracking.

If 4140 must be welded, Atlas gives these minimum precautions:

  • Preheat to 200 to 300 °C (about 390 to 570 °F) and hold that temperature throughout welding.
  • Stress relieve immediately after welding at 500 to 600 °C (about 930 to 1,110 °F).
  • Use low-hydrogen filler and a written welding procedure qualified for the material and condition.

Welding pre-hardened bar also changes its properties near the weld, so the strength in the table above no longer applies there. When a welded part is needed, designers often switch to 4130 or a weldable structural grade.

4140 Equivalent Grades

SystemDesignation
AISI / SAE4140
UNSG41400
EN / DIN42CrMo4 (1.7225); 41CrMo4 is a close equivalent
BS (old British)EN19A
AustralianAS1444 grade 4140
From the voestalpine and Atlas Steels data sheets. “Equivalent” grades overlap but are not identical; check the specification your drawing calls for.

What 4140 Is Used For

Atlas Steels describes 4140 as a steel for medium to highly stressed shafts and components where 1045 carbon steel would not be enough, citing higher yield and fatigue strength, better through-hardening and better impact properties. Typical parts include:

  • Transmission and drive shafts, axles and spindles
  • Small gears, couplings and sprockets
  • Threaded fasteners: bolts, nuts and studs
  • Hydraulic cylinder rods, tool holders and machine parts

For larger sections where the core needs more strength, Atlas suggests 4340 instead, since it hardens deeper and has better impact properties and ductility.

4140 vs Structural Steel (A36 and A992)

People sometimes ask whether 4140 makes a better beam because it is so much stronger. It does not, for practical reasons:

  • Availability: 4140 is sold as round bar, plate and forgings, not as rolled wide flange, channel or angle shapes.
  • Stiffness is the same: nearly all steels have about the same modulus of elasticity, so a 4140 beam would deflect just as much as an A992 beam of the same size. Most beams are sized by deflection or buckling as often as by strength.
  • Weldability and ductility: structural steels such as A36 and ASTM A992 are made to be readily weldable and to stretch a long way before breaking. Hardened 4140 is neither.
  • Code acceptance: building codes and the AISC Specification list the steels approved for structural members. Substituting a different grade needs a licensed structural engineer’s approval.

Frequently Asked Questions

Is 4140 steel stainless?

No. It contains about 1% chromium, far below the roughly 10.5% needed for stainless behavior. It rusts and needs oil, paint, plating or another coating.

What is the difference between 4130 and 4140?

Carbon content. 4130 has about 0.30% carbon and 4140 about 0.40%. 4140 reaches higher strength and hardness after heat treatment; 4130 is easier to weld.

How hard is 4140 steel?

Pre-hardened bar up to about 7 in diameter is typically 269 to 331 HB. Surface hardening can reach about 58 HRC, and nitriding gives a 600 to 650 HV case.

Is 4140 good for knives?

It can hold a usable edge, but it is a general engineering steel rather than a blade steel, so most knife makers choose higher-carbon or tool steels.

Can 4140 be used for structural bolts?

Bolts are bought to a fastener specification, not a raw steel grade. The specification sets the heat treatment, strength and markings. Use the bolt grade on the drawings; our bolt grades guide explains the common markings.

Reference information only, not engineering advice. Disclaimer.

Look up any steel beam size

Search all 339 AISC W, S and HP shapes, compare sizes by depth and work out total weight in seconds.